A flow function connects strength measurements at several consolidation states to a hopper-design assessment.

Illustration of powder in a hopper beside a shear cell and an unnumbered flow-function curve.

Two shear reports on portions of the same powder can show different strengths because the specimens were prepared at different stresses. For a hopper assessment, the useful question is whether the reported points cover the stresses needed for the design and whether differences at a common stress are meaningful.

One powder, several prepared states

Take representative portions from a documented common sampling and handling history. In a shear test, preshear under a selected normal stress prepares a consolidated state; failure measurements at lower normal stresses establish a yield locus for that state. A different preshear level prepares another state, with a potentially different particle contact network, packing, and measured strength. The direction and size of the change must be measured for the powder.

For Schulze’s construction, the major principal consolidation stress σ₁ comes from the Mohr circle tangent to the yield locus and passing through the steady-state preshear point. The unconfined yield strength fc comes from a different circle tangent to the locus and passing through the origin. Thus the applied preshear normal stress and σ₁ are related but are not interchangeable. Several loci give the paired σ₁ and fc values plotted as the flow function [1]. The shear-cell testing guide explains the measurement sequence in more detail.

ffc = σ₁ / fc

With both stresses in the same units, ffc is dimensionless. It describes flowability at that particular consolidation stress and test condition, so one ffc does not represent the whole curve [1].

Choose the range before choosing settings

Define the hopper geometry, fill and discharge conditions, and the longest relevant loaded standstill. Work with the hopper designer and laboratory to establish the range of major consolidation stresses required by the selected design method. Hopper stresses depend on geometry and wall friction as well as the stored material; fill height alone is not a direct laboratory stress setting.

Ask the laboratory to select preshear settings for that range, and request the preshear stresses, yield loci, derived σ₁ and fc pairs, and the tested range. If the returned points miss a design-relevant region, agree additional tests rather than extrapolating. Tester and cell selection affect what can be measured, as explained in the comparison of Jenike and ring shear testers.

Specify sample preparation, moisture, temperature, apparatus, procedure, and time under load. These records make the resulting curve interpretable and help distinguish a stress effect from a change in specimen condition. If loaded restart matters, request time-consolidation data for the relevant hold period: some powders gain strength during storage, while others change little [1].

Compare the reports and use the curve

Points at different σ₁ values describe different states along a flow function; a difference between them alone does not establish a disagreement. Compare fc or ffc at the same reported σ₁ and under comparable conditions. Where the measured points do not coincide, use a justified interpolation within the measured range and retain the underlying points; obtain additional data if the comparison is consequential and remains uncertain.

For a remaining difference, first assess it against applicable method precision or reported uncertainty. Then inspect preparation, environmental exposure, time under load, instrument, cell, and calculation records. If the difference matters to the design, choose a controlled repeat that holds the shared conditions fixed and changes the suspected factor. Agreement on repeat may suggest the original difference was within measurement variation; a persistent difference associated with the changed factor supports further investigation, although mechanisms can coexist.

The Flow Function / ffc Interpreter accepts multiple measured points, calculates ffc for each, and plots the measured flow function. Retain the test conditions with your records; a plotted curve alone does not establish the hopper stress range. The hopper design check carries that flow function into an outlet assessment with wall friction, geometry, and density. Give the designer the measured pairs and flag any missing stress or storage condition before sizing the outlet.

Technical Basis / Sources

Related Reading

Shear Cell Testing for Hopper Design and Powder Flow

Shear Cell Testing for Hopper Design and Powder Flow: Strength and Friction Properties

Explains how yield loci, flow functions, and shear-cell methods characterize consolidated powder for hopper design.

Using Shear-Test Data to Check a Hopper’s Outlet Size and Wall Angle

Using Shear-Test Data to Check a Hopper’s Outlet Size and Wall Angle

Walks through the use of shear and wall-friction data to assess hopper wall angle and outlet dimensions.

Jenike Shear Cell vs Ring Shear Tester: Matching the Method to the Hopper or Silo Decision

Jenike Shear Cell vs Ring Shear Tester: Matching the Method to the Hopper or Silo Decision

Compares the geometry, test sequence, and selection considerations of Jenike and ring shear testers.